Skip to content

THE COURSE / M1 THE SWITCH / M1.4

The gate: the MOS capacitor

After this lesson you can:

  • Say what gathers under a gate in accumulation, depletion and inversion.
  • Explain the threshold voltage, and work out the band bending it takes.
  • Explain why gate oxides got thinner, why they stopped, and what high-k changed.

Loading the lesson…

Sources

  1. C. C. Hu, Modern Semiconductor Devices for Integrated Circuits (Pearson, 2010), chapter 5, "MOS Capacitor" (free from the author). A gate, an insulator such as SiO₂ as thin as 1.5 nm, and the silicon body; aluminium gates before 1970, then heavily doped polysilicon, and from 2008 metal gates and high-k dielectrics again in the most advanced transistors. On a P body: a negative gate gathers holes (accumulation); a positive gate pushes them away, leaving acceptor ions (depletion); more positive, electrons gather at the surface, inverting it to N type (inversion). Threshold: the surface electron density equals the body doping, at a band bending of 2φB = 2(kT/q) ln(Na/ni). Beyond threshold, Qinv = Cox(Vg − Vt), Cox = εox/Tox; the depletion width stops growing. A lone capacitor takes minutes to make its inversion electrons; in a transistor the N+ junctions supply them. A MOS transistor is a MOS capacitor flanked by two PN junctions.
  2. C. C. Hu, Modern Semiconductor Devices for Integrated Circuits (Pearson, 2010), chapter 7, "MOSFETs in ICs—Scaling, Leakage, and Other Topics" (free from the author). Gate oxide thinned from 300 nm at the 10 µm technology to 1.2 nm at 65 nm, roughly in proportion to the line width, to raise the on-current and to control Vt roll-off as the channel shortens. Below 1.5 nm, tunnelling leakage limits it: 1.2 nm of SiO₂ leaks 10³ A/cm², 10 A from 1 mm² of gate, enough to drain a phone's battery in minutes; nitrogen cuts it about tenfold. HfO₂ has k ≈ 24, six times SiO₂'s: 6 nm of HfO₂ gives the capacitance of 1 nm of SiO₂ (an EOT of 1 nm) with leakage several orders of magnitude lower; a thin SiO₂ interfacial layer under it; metal gates, two metals for N and P transistors. SiO₂ breakdown about 7 MV/cm for ten years' operation. Below threshold the current falls exponentially, by ten for every S = η × 60 mV at room temperature (η ≥ 1; e.g. 90 mV at η = 1.5): the subthreshold swing. Vt is defined where Ids = 100 nA × W/L (some companies 200 nA); Ioff, at Vgs = 0, = 100 nA × (W/L) × 10^(−Vt/S). An Ioff of 100 nA per transistor across a hundred million transistors is 10 A in standby. Vt can't be made arbitrarily small; S is lowered by a thinner oxide or a wider depletion layer. Vt rolls off as the channel shortens: short-channel transistors leak more. Moore (1965): devices per chip double every 18 to 24 months; each node shrinks features to 70%, halving the area of a circuit, every two to three years. Table 7–1 (history and ITRS projection): 90 nm (2003) Vdd 1.2 V, 65 nm 1.1, 45 nm 1.0, 32 nm 1.0, 22 nm (2013) 0.9 V; strained silicon from 90 nm, high-k/metal gate from 45 nm, immersion lithography at 32 nm, a new structure at 22 nm. Strain: SiGe grown in trenches beside a PFET's gate compresses its channel and raises hole mobility. Vt roll-off: in a short channel the drain lowers the source–channel barrier (drain-induced barrier lowering), so less gate voltage is needed; roll-off ∝ (Vds + 0.4 V) e^(−L/ld), ld ∝ (Toxe Wdep Xj)^(1/3); minimum L several times ld. Even with a thin oxide the drain controls leakage paths below the surface, far from the gate: ultra-thin bodies and multigate transistors remove them. Random dopant fluctuation: the number and place of dopant atoms in a small transistor varies, and with it Vt. Designers get two or three Vts to choose from.